How Steel Castings Are Accepted: Reference Radiographs, Quality Levels and the Purchase Order
Castings are not judged by a welding code. The purchase order or product specification names a reference standard and a level for each method: severity levels against ASTM E446, E186 or E280 reference radiographs by discontinuity category, an ASTM A609 quality level for ultrasonics, an ASTM A903 acceptance level for magnetic particle and penetrant, or the MSS SP practices for valve and fitting castings.
None of those standards sets a universal pass mark. ASTM E446 says plainly that purchaser and manufacturer select, by mutual agreement, the discontinuity classes that will represent minimum acceptability, and ASTM A609 says the same of its ultrasonic quality levels. The level can change across one casting: a valve body may carry a strict level at the weld ends and seating areas and a looser one elsewhere, recorded on a nondestructive test drawing. Porosity is one category among several, so a question about the porosity acceptance level has no answer until the specification, the method and the zone are known. In a pressure vessel the vessel code adds a second layer, because ASME Section VIII Division 1 ties the allowable stress for a casting to how thoroughly it was examined. The table below maps each method to its reference document, and the sections explain how the levels are read and written into an order.
Source: ASTM E446-15 (castings up to 2 in.), ASTM E186 (2 to 4-1/2 in.) and ASTM E280-21 (4-1/2 to 12 in.) reference radiographs; ASTM E2868 digital reference images; ASTM E1030 (radiographic examination of metallic castings); ASTM A609/A609M-12 (Reapproved 2023); ASTM A903/A903M-99 (Reapproved 2024); ASTM E709 and E165/E165M; MSS SP-53, SP-54, SP-55, SP-93 and SP-94; ASME BPVC Section VIII Division 1 (2023 edition), UG-24 and Mandatory Appendix 7. The edition named in the purchase order or product specification governs.
| Method and scope | Technique document | Acceptance reference | How the level is expressed | Who sets the level |
|---|---|---|---|---|
| Radiography, sections up to 2 in. (50.8 mm) | ASTM E1030 or ASME Section V Article 2 | ASTM E446 reference radiographs | Six graded categories (A, B, Ca, Cb, Cc, Cd) at severity levels 1 to 5; D, E, F and G ungraded | Purchaser and manufacturer by agreement |
| Radiography, sections 2 to 4-1/2 in. | ASTM E1030 or ASME Section V Article 2 | ASTM E186 reference radiographs | Gas porosity, sand and slag, and shrinkage types graded by severity level; cracks, hot tears and inserts ungraded | Purchaser and manufacturer by agreement |
| Radiography, sections 4-1/2 to 12 in. (114 to 305 mm) | ASTM E1030 or ASME Section V Article 2 | ASTM E280 reference radiographs | A, B and Ca to Cc at severity levels 1 to 5; D, E and F as recognition guides | Purchaser and manufacturer by agreement |
| Ultrasonic, carbon, low-alloy and martensitic stainless castings | ASTM A609 Procedure A (flat-bottomed holes) or Procedure B (back wall) | ASTM A609 quality levels 1 to 7 | Area and length of response at or above the DAC, or of 75% back-reflection loss | Purchaser, for the whole casting or portions of it |
| Magnetic particle and penetrant | ASTM E709 and E165/E165M | ASTM A903 acceptance levels | Limits on relevant linear and nonlinear indications; relevant means over 1/16 in. (1.6 mm) | Purchaser, with an NDT drawing where levels vary by location |
| Valve, flange and fitting castings | Method practice named by the product standard | MSS SP-53 (MT), SP-54 (RT), SP-55 (visual), SP-93 (PT), SP-94 (UT) | Each practice's own reference images and limits | Product standard and purchase order |
| Pressure-retaining castings in a Division 1 vessel | As the material specification and Appendix 7 require | ASME Section VIII Division 1 UG-24 and Mandatory Appendix 7 | A casting quality factor applied to allowable stress | Vessel designer and manufacturer |
Why castings need their own acceptance language
A weld has a known geometry and a short list of likely flaws, and the welding codes judge them by length against thickness. A casting can hold discontinuities anywhere in its volume, and its typical ones come from solidification rather than from a welder: gas porosity, sand and slag inclusions, shrinkage in several forms, hot tears, cracks, and unfused chills or chaplets. Those shapes do not translate into the length limits of UW-51 or Table 341.3.2, so casting acceptance grew up around comparison with reference images and around quality levels agreed between buyer and foundry.
That approach has a consequence worth understanding before writing an order. Researchers working with the Steel Founders' Society of America have described the reference radiographs as workmanship standards that are unrelated to performance, and found that adjacent shrinkage levels are hard to tell apart. A severity level states how the casting compares with an agreed picture; it does not, by itself, state that the part will carry its load. Choosing the level is therefore an engineering decision for whoever owns the design, and the inspector's job is to apply it consistently. Our casting quality control guide covers how the methods fit together across a foundry's process.
Reading the ASTM reference radiographs: categories and severity levels
Three ASTM standards cover steel castings by section thickness. E446 covers sections up to 2 in. (50.8 mm), E186 covers 2 to 4-1/2 in., and E280 covers heavy-walled castings of 4-1/2 to 12 in. (114 to 305 mm). Each is a set of physical reference radiographs, purchased separately as an adjunct, and the written standard explains how to use them. E446 notes that it and E186 overlap in severity levels within the same energy range and allows E186 levels to be used when the purchaser-supplier agreement says so.
Within each set, discontinuities are sorted into categories. In E446 the graded categories are A for gas porosity, B for sand and slag inclusions, and four shrinkage types under C: Ca linear, Cb feathery, Cc sponge and Cd combined. Each graded category has reference images at severity levels 1 to 5, with level 1 the least severe. Categories D (crack), E (hot tear), F (insert) and G (mottling) are ungraded illustrations. E280 grades A, B and shrinkage types Ca to Cc at levels 1 to 5, and its D, E and F plates act as recognition guides.
Because the ungraded categories have no levels to choose from, a specification normally says how they are treated, and many treat cracks, hot tears and inserts as unacceptable outright. The interpreter compares the production radiograph with the reference image for the right category and thickness and decides whether the indication is no worse than the specified level. Misjudging the category is as serious as misjudging the level: calling shrinkage gas porosity, or a hot tear a shrinkage line, moves the indication into a different column of the order. Our guide to identifying shrinkage cavities in castings shows what separates them on film.
Film, digital images and the radiographic technique
The reference radiographs were made on film. E446 states that its images are not intended to illustrate discontinuities for digital radiography, and directs digital work on castings up to 2 in. to the digital reference image standard E2868. A contract that moves a foundry from film to digital detectors without changing the acceptance reference has quietly changed the basis of comparison, and the order should name the digital reference set and the agreed equivalence. E446 also notes that its adjunct radiographs remain valid regardless of when they were produced.
Technique is a separate document from acceptance. ASTM E1030 is the practice for radiographic examination of metallic castings, and ASME Section V Article 2 serves the same purpose where a pressure code governs. Either sets how exposures, image quality indicators and coverage are handled; neither tells the interpreter whether an indication passes. For readers in the United States, note that Atlantis does not perform radiography in the United States; where the code allows, ultrasonic testing is used for volumetric examination, and our ASNT Level III can review radiographs and RT procedures produced by a licensed contractor.
Porosity in castings: what a severity level actually limits
Searches for a casting porosity acceptance level usually come from someone holding a radiograph or a sectioned part and looking for a number. The honest answer is that the number lives in the order. Gas porosity is Category A in the reference radiographs, and the acceptance level is the severity level the order assigns to Category A for that zone and thickness. Two buyers of the same casting can specify different levels, and one buyer can specify different levels in different parts of the same casting.
What the order should not do is borrow a porosity limit from somewhere else. The rounded-indication charts in ASME Section VIII Appendix 4 and the porosity rules of API 1104 were written for welds, at weld thicknesses and against weld service, and they have no standing on a casting unless the specification expressly invokes them. The same goes for the reverse: a casting severity level does not belong in a welding procedure.
Shrinkage deserves more care than porosity because it sits in heavy sections and at changes of section, where stresses are often highest, and because its forms grade differently. Where porosity is found by ultrasonics rather than radiography, the decision is made under the ultrasonic quality level, not by estimating a radiographic severity. Our page on detecting internal porosity in castings discusses what each method can and cannot show.
Ultrasonic acceptance under ASTM A609
A609 covers pulse-echo ultrasonic examination of heat-treated carbon, low-alloy and martensitic stainless steel castings; austenitic stainless castings are outside its scope. Procedure A calibrates on a series of test blocks containing flat-bottomed holes and builds a distance-amplitude curve, with supplementary angle-beam requirements. Procedure B calibrates on the back wall reflection from a series of solid blocks.
Acceptance quality levels are established between purchaser and manufacturer on one or more criteria: no indication at or above the DAC over an area larger than the level allows, no loss of back reflection of 75% or more caused by a discontinuity over that area, no continuous DAC-level response longer than the level's maximum length, or other agreed criteria. The standard's table runs from quality level 1, the most demanding, at 0.8 in.² (5 cm²) and 1.5 in. (40 mm) maximum length, to quality level 7 at 16 in.² (100 cm²) and 6.9 in. (175 mm). The purchaser specifies the level for the whole casting or for portions of it, and identifies sections that need longitudinal-beam, dual-element or supplementary angle-beam examination.
Two points trip contractors. The area is the casting surface area over which the qualifying response is maintained, not the reflector's estimated size. And a level written for the whole casting can be impossible to apply near complex geometry, so the order should map zones. See ultrasonic testing of castings and forgings for how this is planned on site.
Surface acceptance under ASTM A903
A903 is a specification of acceptance criteria for steel castings examined by magnetic particle or liquid penetrant methods, with technique taken from guides such as ASTM E709 for magnetic particle and ASTM E165 for penetrant. It applies when a document states that surface acceptance shall be to A903.
Only indications whose major dimension exceeds 1/16 in. (1.6 mm) are relevant. A903 classes an indication as linear when its length is equal to or greater than three times its width, and nonlinear when it is less. That boundary differs slightly from the ASME surface-examination appendices, which call an indication linear only when its length is more than three times its width, so an indication exactly three times as long as it is wide is linear under A903 and rounded under the ASME vessel rules. The point matters when one foundry supplies both a valve purchaser and a vessel fabricator.
The order names the acceptance level and the extent of examination, and where different levels apply at different locations, A903 calls for a nondestructive test drawing identifying the levels and locations to accompany the inquiry and order. For site practice on cast parts, see magnetic particle inspection of castings and forgings and penetrant testing of castings.
Valve and fitting castings: the MSS practices
Valves, flanges and fittings bring their own family of quality standards from the Manufacturers Standardization Society: SP-53 for magnetic particle examination, SP-54 for radiography, SP-55 for visual evaluation of surface irregularities, SP-93 for liquid penetrant and SP-94 for ultrasonic examination of ferritic and martensitic castings. Valve and fitting purchase specifications, and some product standards, cite them so that a buyer can call for, say, radiography and magnetic particle examination of critical areas without writing acceptance criteria from scratch.
The MSS practice cited is the acceptance reference for that examination, and it sits alongside whatever the product standard and the purchase order add. Contractors run into trouble when they substitute a general ASTM level for the MSS practice the order names, or apply a weld acceptance table to a cast valve body because the valve sits in a piping system built to B31.3. The piping code governs the welds that join the valve to the line; the casting is accepted to its own documents.
MSS SP-54 shows how closely these practices lean on the ASTM sets. Its 2013 edition describes itself as providing methods and acceptance standards for the film method of radiographic examination of steel castings, and it covers both the first examination of a casting and the examination of casting repairs. Interpretation follows wall thickness: E446 up to 2 in., E186 from 2 in. to under 4-1/2 in., and E280 from 4-1/2 to 12 in. Like the ASTM documents it is voluntary until an inquiry, contract or order names it, so a valve buyer who wants SP-54 applied has to say so in writing.
Castings in ASME pressure vessels: UG-24 and Appendix 7
Section VIII Division 1 does not put casting acceptance in its welding paragraphs. UG-24 instead applies a casting quality factor to the allowable stress of a cast part, and the factor permitted rises with the examination performed beyond the minimum of the material specification. The higher factors call for the additional examinations of Mandatory Appendix 7, Examination of Steel Castings, which bring radiographic or ultrasonic and surface examination into the vessel code's own rules.
The effect is that the vessel designer, not the inspector, decides how much examination a casting needs, by choosing the factor the design calculation uses. If the examination later performed does not support that factor, the thickness calculation no longer stands. Read UG-24 and Appendix 7 in the edition the vessel is built to before quoting any factor or examination requirement, and see the Section VIII Division 1 acceptance criteria guide for the weld side of the same vessel.
Sections that cross a reference-set boundary
Severity levels are read from the reference set that matches the section being examined, not the heaviest wall of the casting. A valve body with a 1-1/2 in. neck and a 3 in. body straddles E446 and E186, and a large pump casing can need E186 and E280 on different parts of the same casting. The order or the NDT drawing should say which set applies to which zone, and the interpreter should record the measured section thickness at each film location so that a reviewer can check the choice of reference afterwards.
If the order relies on the E446 and E186 overlap described earlier, the agreement belongs in writing beside the levels, because an auditor reading a thin-section radiograph judged against E186 will otherwise call it the wrong reference. The same discipline applies to castings whose section changes sharply at a flange or boss: a film that covers both thicknesses is evaluated against the set for each part of the image, not averaged.
Who interprets the films and who signs the acceptance
Interpretation is a Level II or Level III task under the employer's written practice. The interpreter needs the correct adjunct set in hand and should view it under the same conditions as the production films, since the whole decision is a visual comparison. At the foundry this is normally the first decision, and many purchase orders reserve the purchaser's right to review films or witness examination before the casting ships.
When foundry and purchaser disagree about a film, the outcome depends on what the order says about who decides, which is why the order should name the accepting party for each method instead of leaving it to the first dispute. A Level III review that records the category, the level and the reference set for each film gives both sides the same written basis to argue from, and it turns a disagreement about pictures into a check of documented choices.
Weld repairs on castings and how they are re-examined
Foundries repair castings by welding as a routine part of production, and the product specification controls how. In ASTM A216 as issued in 1993 and reapproved in 2003, the edition quoted here, repairs are made with procedures and welders qualified to ASTM A488, and where magnetic particle or radiographic examination has been specified as a supplementary requirement, repairs are inspected to the same quality standards as the casting itself. Where radiography is specified, repairs are radiographed on castings that leaked on hydrostatic test, where the cavity prepared for welding is deeper than 20 percent of the wall or 1 in. (25 mm), whichever is smaller, or where it is larger than about 10 in.² (65 cm²). Repairs of that size also bring post-weld stress relief or heat treatment, and a further supplementary requirement covers examination of the prepared cavity itself by magnetic particle or penetrant methods to E709 or E165.
ASTM has revised A216 several times since, most recently as A216/A216M-26, and later editions may word or place these rules differently, so read the repair clauses in the edition the order invokes. For the buyer, the practical decisions are whether repair welding is allowed at all in critical zones, whether larger repairs need notice or approval before welding starts, and how the repair locations are mapped and reported. A repaired area judged only by the method that found the original defect can hide a weld flaw the other method would show, so the order should say which methods apply to repairs.
When radiography and ultrasonics disagree
A casting examined by both methods can pass one and fail the other, because the methods respond to different features. A planar shrinkage line can give a strong ultrasonic response at the right beam angle and only a faint image on film, while scattered gas porosity can grade poorly on a radiograph yet stay below the ultrasonic recording level. Each result is judged by its own acceptance document, a severity level for the film and an A609 quality level for the ultrasonic data, and neither result converts into the other.
The order should therefore state whether both methods must pass, or which method governs a given zone. Without that statement, expect the stricter result to be applied and the casting to be held for a decision, which is the slowest possible way to find out that the specification was incomplete.
Writing the casting NDT requirement and the report
A workable order or specification states, for each method: the reference document and its edition; the technique document; the zones or critical areas, shown on an NDT drawing; the level for each graded category or quality level for each zone, and how ungraded categories are treated; whether film or digital reference images apply; whether repair welding is permitted, to what procedure, and how repairs are re-examined; and who accepts the result.
The report should identify the casting by pattern, heat and serial number and the drawing revision; list the areas examined and any areas not covered; state the technique and reference used; and record, for each relevant indication, its location, category or classification, the level assigned and the decision. Recording the level that was assigned, not just accept, lets the buyer see how close a part came to rejection, which is useful when deciding whether a foundry's process needs attention. Report templates in Atlantis ERP NDT reports can carry the reference and level fields so they are never left blank.
Where Atlantis fits
In the United States our technicians perform ultrasonic, magnetic particle, penetrant and visual examination of castings at the client's or foundry's site, to the reference and level the order names. Our ASNT NDT Level III writes casting examination procedures, prepares the zone drawings and acceptance clauses that turn a purchase order into something an inspector can apply, and reviews contractor radiographs against E446, E186 or E280. See NDT procedure development and NDT Level III consulting, and the NDT acceptance criteria hub for how castings sit alongside the welding codes.
What is the acceptance level for porosity in castings?
There is no universal level. Gas porosity is Category A in the ASTM reference radiographs, and the acceptance level is the severity level the purchase order or product specification assigns to Category A for that zone and thickness, from level 1 (least severe) to level 5. Porosity limits written for welds, such as ASME Appendix 4, do not apply to castings unless the specification invokes them.
What is the difference between ASTM E446, E186 and E280?
Section thickness. E446 provides reference radiographs for steel castings up to 2 in. (50.8 mm), E186 for 2 to 4-1/2 in., and E280 for heavy-walled castings of 4-1/2 to 12 in. (114 to 305 mm). Each grades gas porosity, sand and slag, and shrinkage types by severity level, with cracks, hot tears and inserts shown as ungraded examples.
Are cracks and hot tears graded in the ASTM casting reference radiographs?
No. In E446, E186 and E280 cracks (Category D), hot tears (E) and inserts (F) are ungraded illustrations or recognition guides, not severity levels. The specification decides how they are treated, and many purchase specifications reject them outright, so a crack-like indication on a casting radiograph is normally a reject or a repair.
What do ASTM A609 quality levels mean?
They are seven ultrasonic acceptance levels for carbon, low-alloy and martensitic stainless castings. Each limits the casting surface area, and the length, over which a response at or above the DAC or a back-reflection loss of 75% or more may continue: from 0.8 in.2 and 1.5 in. at level 1 to 16 in.2 and 6.9 in. at level 7. The purchaser chooses the level for each portion of the casting.
How is a linear indication defined for steel castings under ASTM A903?
An indication whose length is equal to or greater than three times its width is linear; anything shorter relative to its width is nonlinear. Only indications with a major dimension over 1/16 in. (1.6 mm) are relevant. The ASME vessel appendices draw the line at more than three times, so an indication at exactly three to one is classified differently under the two documents.
Can ASTM E446 reference radiographs be used for digital radiography?
E446 states that its film reference radiographs are not intended to illustrate discontinuities for digital radiography and points digital examination of castings up to 2 in. to ASTM E2868, the digital reference image standard. A purchase order that allows digital imaging should name the digital reference set and the agreed basis of comparison.
Need this applied on your job?
Atlantis writes and reviews procedures to the codes you work under, and provides the inspection and the training.