RT and UT Acceptance Criteria for Section VIII Division 1 Pressure Vessel Welds
Section VIII Division 1 sets radiographic acceptance in UW-51 for fully radiographed joints and UW-52 for spot radiography. UW-51 rejects any crack or zone of incomplete fusion or penetration, and any elongated indication longer than 1/4 in. for t up to 3/4 in., 1/3t for t from 3/4 to 2-1/4 in., or 3/4 in. above that. Mandatory Appendix 4 governs rounded indications.
Spot radiography under UW-52 is judged differently: cracks and incomplete fusion or penetration still reject the spot, a slag inclusion or cavity is rejected when longer than 2/3t, though anything under 1/4 in. passes and nothing over 3/4 in. does, and rounded indications are not evaluated. Ultrasonic acceptance depends on why the ultrasonic examination is being done. Where Division 1 itself calls for it, or the Manufacturer chooses it for a repair, Mandatory Appendix 12 applies: cracks, lack of fusion and incomplete penetration are unacceptable at any length, and other indications above the reference level are rejected beyond the same three thickness-based lengths as UW-51. Where ultrasonics replaces radiography altogether under UW-51(a)(4), for welds whose thinner member is 1/4 in. or thicker, the method and acceptance come from paragraph 7.5.5 of Division 2, with computer-based data acquisition and flaw-size criteria. Surface examinations are judged by Appendices 6 and 8, and finished-weld visual requirements sit in UW-35.
Source: ASME BPVC Section VIII Division 1 (2023 edition; the UW-51 and UW-52 wording was also read in the 2019 edition): UW-11, UW-12, UW-35, UW-38, UW-51 including UW-51(a)(4), UW-52, Mandatory Appendix 4 (rounded indications), Mandatory Appendices 6 and 8 (magnetic particle and penetrant) and Mandatory Appendix 12 (ultrasonic examination of welds); Section VIII Division 2 paragraph 7.5.5; ASME BPVC Section V Articles 2, 4, 6, 7 and 9. Values are in U.S. customary units with SI as the code prints them; confirm them against the edition your construction code or contract invokes.
| Indication or situation | Limit or rule | Clause | Note for the reviewer |
|---|---|---|---|
| Crack, incomplete fusion or incomplete penetration (full RT) | Unacceptable at any length | UW-51(b) | No length allowance exists for these |
| Elongated indication, t up to 3/4 in. (19 mm) | Rejected if longer than 1/4 in. (6 mm) | UW-51(b) | Take t from the clause's definition of weld thickness |
| Elongated indication, t from 3/4 in. to 2-1/4 in. (57 mm) | Rejected if longer than 1/3t | UW-51(b) | A 1-1/2 in. weld allows 1/2 in. |
| Elongated indication, t over 2-1/4 in. | Rejected if longer than 3/4 in. (19 mm) | UW-51(b) | The limit stops growing with thickness |
| Aligned group (full RT) | Rejected if aggregate length exceeds t in a length of 12t, unless successive imperfections are more than 6L apart | UW-51(b) | L is the longest imperfection in the group |
| Rounded indications (full RT) | Within the Appendix 4 size rules and charts for the thickness | Mandatory Appendix 4 | Charts are full-scale 6 in. (150 mm) lengths |
| Spot RT: slag inclusions or cavities | Rejected if any one is longer than 2/3t; under 1/4 in. (6 mm) always passes and over 3/4 in. (19 mm) never does; a line of them may total t in 6t when the longest are 3L apart | UW-52 | Each spot at least 6 in. (150 mm) long; rounded indications not evaluated |
| Manual UT where Division 1 calls for UT, or UT of a repair | Cracks, lack of fusion, incomplete penetration rejected at any length; other indications above reference level rejected beyond the UW-51 lengths | Mandatory Appendix 12 | Amplitude plus length; responses over 20% of the reference level are investigated |
| UT in place of RT, thinner member 1/4 in. (6 mm) or more | Acceptance by the Division 2 method the paragraph invokes | UW-51(a)(4); Division 2, 7.5.5 | Encoded, computer-based data; not Appendix 12 |
Start with the joint: which acceptance clause applies
Before anyone reads a radiograph on a Division 1 vessel, the inspection plan has to say how each joint was designed. The extent of radiography follows from the joint efficiency the designer chose. A joint designed for full radiography is examined to UW-11 and judged to UW-51. A joint whose efficiency was taken from the spot-radiography column of Table UW-12 is sampled and judged to UW-52. A joint designed with no radiography carries no code-required radiographic acceptance; if an owner wants it radiographed anyway, the purchase specification has to name the standard. The efficiency table and the UW-11 triggers are explained on our Section VIII Division 1 construction page; this guide picks up at the accept-or-reject decision.
The two radiographic clauses are not interchangeable. A spot film read to UW-51 drags in the rounded-indication charts, which UW-52 does not apply, and a fully radiographed seam read to the spot rules has been accepted against a looser standard than its design assumed. The nameplate carries the vessel's radiography marking, RT 1 to RT 4 under UG-116, and the Manufacturer's Data Report records the examination, so a reviewer can establish which clause should have been used before judging whether it was used correctly.
UW-51: limits for fully radiographed joints
UW-51 opens by sending the technique to Section V Article 2. Image quality, IQI selection and density are technique questions, and the clause accepts demonstrated density and visibility of the specified IQI hole or wire as evidence that Article 2 was met. Only then does it list the indications that make a weld unacceptable. Any indication characterised as a crack or as a zone of incomplete fusion or penetration is rejected outright. Elongated indications such as slag lines are limited by length against the weld thickness t: 1/4 in. (6 mm) where t is up to 3/4 in. (19 mm), one third of t from 3/4 in. to 2-1/4 in. (57 mm), and 3/4 in. (19 mm) above 2-1/4 in.
Aligned indications are judged as a group. A row is rejected when the lengths add up to more than t within a weld length of 12t, unless the gap between successive imperfections is more than six times the length of the longest one in the group, in which case they are assessed separately. Rounded indications on a fully radiographed joint go to Mandatory Appendix 4. Take t from the clause's own definition of weld thickness before applying any limit; measuring it over the cap overstates every allowance. Technique detail is on our Section V Article 2 page.
A worked example shows how quickly the numbers move. On a 1/2 in. shell seam the longest acceptable elongated indication is 1/4 in., and a line of slag whose pieces total more than 1/2 in. within any 6 in. of weld is rejected unless the pieces are far enough apart to be treated individually. On a 1-1/2 in. seam the individual limit rises to 1/2 in. and the aligned-group window grows to 18 in.
Rounded indications: how the Appendix 4 charts work
Mandatory Appendix 4 covers rounded indications, porosity and similar compact indications, on joints that must be fully radiographed. It first decides which rounded indications count. Below a size that depends on thickness they are not relevant: one tenth of t where t is under 1/8 in., 1/64 in. from 1/8 in. to 1/4 in. inclusive, 1/32 in. above 1/4 in. up to 2 in., and 1/16 in. above 2 in. Relevant indications are then limited individually. The largest permitted is 1/4t or 5/32 in., whichever is smaller, except that an isolated indication 1 in. or more from its neighbours may reach 1/3t or 1/4 in., whichever is smaller, rising to 3/8 in. for isolated indications in welds over 2 in.
Concentration is judged against the charts. Each chart represents a full-scale 6 in. (150 mm) length of radiograph for one thickness range, shows the maximum acceptable concentration of rounded indications, and must not be enlarged or reduced; the dot patterns illustrate density, not a pattern a film has to match. Clustered indications may be up to four times as concentrated as the random-indication charts in a local area, provided the cluster is no longer than 1 in. or 2t, whichever is less. Rounded indications in a line are acceptable when their diameters add up to less than t in a length of 12t, and for welds thinner than 1/8 in. the appendix caps the count at 12 rounded indications in a 6 in. length.
In practice the reviewer measures each rounded indication, discards those below the relevance size, checks the largest against the size limits, checks any aligned rows, and only then places the film beside the chart for the governing thickness range. Because the charts are drawn at full scale, a digital image has to be viewed at a known scale before it is compared. Appendix 4 does not apply to spot-radiographed welds, which surprises more fabricators than it should.
UW-52 spot radiography: acceptance and the retest sequence
Spot radiography is a sampling plan. UW-52 calls for at least one spot for each 50 ft (15 m) increment of weld, or fraction of one, on welds whose joint efficiency was taken from the spot column of UW-12, with sampling kept separate for each welder or welding operator so that one person's work cannot hide behind another's. The Inspector chooses the spot locations once the increment is complete, and each spot radiograph must be at least 6 in. (150 mm) long. The clause itself says spot radiography is an aid to quality control that does not guarantee a predetermined quality level throughout the weld, which is why its acceptance rules and its follow-up rules have to be read together.
The spot acceptance standard is shorter than UW-51. Cracks and zones of incomplete fusion or penetration reject the spot. Slag inclusions and cavities reject it when any single indication is longer than 2/3t. UW-52 then adds three rules of its own. Several acceptable imperfections lying in line still pass if their longest dimensions add up to no more than t in a length of 6t and the longest of them are separated by at least 3L of acceptable weld metal, L being the length of the longest. No acceptable imperfection may be longer than 3/4 in. (19 mm), and one shorter than 1/4 in. (6 mm) is acceptable whatever the plate thickness. None of these values belongs in a UW-51 evaluation, and none of the UW-51 values belongs here. Rounded indications are not a factor in the acceptability of a spot-radiographed weld.
When a spot fails, the increment is not rejected straight away. Two further spots are taken in the same increment, at locations away from the first. If both are acceptable, the whole increment is accepted, provided the defect shown on the first radiograph is repaired and the repair examined. If either additional spot fails, the entire increment is rejected: the weld is removed and the joint rewelded or, at the fabricator's option, the whole increment is radiographed and only the defective welding corrected, with the repaired or rewelded work then examined as UW-52 directs. An inspection plan that stops at repairing and re-shooting the failed spot has skipped the step that protects the rest of the increment.
Ultrasonic acceptance: three routes, three sets of rules
Most confusion about ultrasonic acceptance on Division 1 vessels comes from treating every UT examination alike. There are three distinct cases. The first is ultrasonic examination used instead of radiography under UW-51(a)(4), available for welds whose thinner member is 1/4 in. (6 mm) or thicker. That paragraph does not point to Appendix 12; it requires the examination to meet paragraph 7.5.5 of Division 2, so the Certificate Holder needs the Division 2 text. The Section V Article 4 rules behind it call for automated or semi-automated scanning with computer-based data acquisition and analysis, and acceptance is fracture-mechanics based: indications are sized and compared with permitted flaw dimensions rather than judged by echo height. Manual pulse-echo scanning is not a substitute on this route.
The second case is ultrasonic examination that Division 1 itself requires or allows in particular situations, such as a final closure seam that cannot be radiographed. Here Mandatory Appendix 12 applies and manual scanning is acceptable. Its standard is amplitude plus length: indications characterised as cracks, lack of fusion or incomplete penetration are unacceptable whatever their length, and any other indication exceeding the reference level is rejected if it is longer than 1/4 in. for t up to 3/4 in., 1/3t from 3/4 in. to 2-1/4 in., or 3/4 in. above 2-1/4 in. Any imperfection producing a response greater than 20 percent of the reference level must be investigated until its shape, identity and location are known, and the Manufacturer keeps a record of reflections from uncorrected areas that exceed 50 percent of the reference level.
The third case is a repair. UW-51 lets the Manufacturer examine a repaired area ultrasonically to Appendix 12 instead of re-radiographing it; for material thicker than 1 in. (25 mm) the user's concurrence is needed, and the ultrasonic examination is noted under Remarks on the Manufacturer's Data Report. A Level III reviewing UT records on a vessel should therefore ask first which of the three routes was used, because calibration, recording and the accept-reject logic all follow from that answer. Our Section V Article 4 page covers the technique, and ultrasonic acceptance criteria by code compares Appendix 12 with the piping and structural codes.
Surface and visual examination on the same vessel
Magnetic particle and penetrant examinations on Division 1 vessels are judged by Mandatory Appendices 6 and 8, which share one rule set built on a relevance threshold, a linear-versus-rounded classification and a line-of-four rule. They are explained in full in our guide to PT and MT acceptance in Section VIII; the technique comes from Section V Articles 6 and 7.
Visual acceptance for finished butt joints sits in UW-35: complete penetration and fusion, a weld surface that allows the required examinations to be interpreted, and limits on undercut and on reinforcement by thickness. The visual technique itself is in Section V Article 9. Surface condition is more than cosmetic on a radiographed or ultrasonically examined joint. Ripples and grooves that mask an indication on the image or disturb the ultrasonic beam make the volumetric result unreliable, which is why UW-35 ties the surface requirement to interpretation rather than appearance.
Recording indications and handling repairs
Accept-or-reject decisions are only as good as the measurements behind them. Elongated indications are measured along their length on the image, or by the ultrasonic length-sizing method the procedure names, and the thickness used for each limit should be written on the report beside the decision, because a reviewer cannot check a 1/3t limit without knowing t. Where thickness changes across a joint, as at a tapered head-to-shell seam, the report should say which thickness was used and why.
Relevant indications that pass should still be recorded with location and size. On a vessel that will later be inspected under API 510, that baseline is what lets an in-service examiner tell a fabrication indication from new damage. Rejectable indications are removed and repaired under UW-38, and the repair is re-examined by the method that found the defect, or ultrasonically to Appendix 12 where UW-51 allows that option. On spot-radiographed welds the repair is re-examined as UW-52 directs.
Errors Level IIIs find in vessel procedures and reports
The same handful of problems appears in contractor documents again and again. Procedures cite Section V Article 2 or Article 4 as the acceptance standard. Reports on spot films apply Appendix 4 and reject sound welds for porosity that UW-52 does not evaluate, or apply the spot rules to a seam the data report shows as fully radiographed. Thickness is taken over the cap. Ultrasonic procedures written for UW-51(a)(4) quote Appendix 12 acceptance and use manual scanning, which is the wrong rule set and the wrong technique. Repairs in material over 1 in. thick are accepted by UT with no record of the user's concurrence.
Others are subtler. Rounded-indication charts are printed or displayed at a scale other than full size. Pinpoint indications below the relevance size are counted toward chart concentration. Aligned rows are never checked because each indication was individually acceptable. The edition of Division 1 is not named, so nobody can confirm which version of a limit was applied. Each of these can be prevented at the procedure stage by an acceptance clause that names the paragraph, the edition and the measurement method, which is the core of NDT procedure development.
How Division 1 compares with Section I, Division 2 and the piping codes
The UW-51 length limits are familiar enough that people assume they apply everywhere. They do not. Power boilers are built to Section I, which carries its own examination requirements and acceptance standards in Part PW and its own routes for replacing radiography with ultrasonics; see Section I weld acceptance criteria. Division 2 vessels follow Part 7 of that division. Process piping attached to the vessel is judged by B31.3 and power piping by B31.1, each with its own tables and paragraphs, as the acceptance criteria by code hub sets out.
Once the vessel is in service, Division 1 acceptance stops being the last word. Inspection, repair and alteration fall under API 510 or the National Board Inspection Code, and the owner's Authorized Inspector decides on the results. An indication that would fail UW-51 on a new seam may be repaired, monitored or evaluated by the owner's engineer. Atlantis does not perform fitness-for-service assessments; our part is to size and describe the indication accurately so that the engineer's decision rests on sound data.
Where Atlantis fits
Atlantis's ASNT NDT Level III prepares Division 1 radiographic and ultrasonic procedures whose acceptance clauses name the paragraph and edition, qualifies and demonstrates ultrasonic techniques, and reviews contractor radiographs and UT records against UW-51, UW-52 and Appendix 12 before they reach the Authorized Inspector. See procedure qualification and demonstration.
In the United States our technicians perform ultrasonic weld inspection, magnetic particle, penetrant and visual examination at the fabricator's or owner's site. Atlantis does not perform radiography in the United States; where the code allows, ultrasonic testing is used for volumetric examination, and our ASNT Level III can review radiographs and RT procedures produced by a licensed contractor. Technicians preparing to apply these limits can work through UT training, and report templates that carry the acceptance clause can be set up in Atlantis ERP NDT reports.
What are the RT acceptance criteria in ASME Section VIII Division 1?
For fully radiographed joints, UW-51 rejects any crack or zone of incomplete fusion or penetration; elongated indications longer than 1/4 in. for t up to 3/4 in., 1/3t from 3/4 in. to 2-1/4 in., or 3/4 in. above 2-1/4 in.; aligned groups totalling more than t in a length of 12t unless the gaps exceed 6L; and rounded indications beyond Mandatory Appendix 4. Spot-radiographed welds are judged to UW-52 instead.
What are the UW-52 acceptance criteria for spot radiography?
A spot is rejected for any crack or zone of incomplete fusion or penetration, or for a slag inclusion or cavity longer than 2/3t. Imperfections in line pass when their total is no more than t in a length of 6t and the longest are at least 3L apart; no acceptable imperfection may exceed 3/4 in., and any shorter than 1/4 in. is accepted at every thickness. Rounded indications play no part, and each spot radiograph must be at least 6 in. (150 mm) long.
Can ultrasonic testing replace radiography on a Section VIII Division 1 vessel?
Yes. UW-51(a)(4) allows ultrasonic examination in place of radiography for welds whose thinner member is 1/4 in. (6 mm) or thicker. The examination must meet paragraph 7.5.5 of Division 2, which relies on automated or semi-automated scanning with computer-based data acquisition and on fracture-mechanics-based acceptance of sized flaws. That is a different rule set from manual ultrasonic examination to Mandatory Appendix 12.
What does Mandatory Appendix 12 say about UT acceptance?
Appendix 12 judges indications by amplitude and length, after investigating every response above 20 percent of the reference level. Cracks, lack of fusion and incomplete penetration are unacceptable at any length. Any other indication exceeding the reference level is rejected when longer than 1/4 in. for t up to 3/4 in., 1/3t from 3/4 in. to 2-1/4 in., or 3/4 in. above 2-1/4 in. It applies where Division 1 calls for ultrasonic examination, such as a closure seam that cannot be radiographed, and to ultrasonic examination of repairs.
Do rounded indications count on spot-radiographed welds?
No. Under UW-52, rounded indications are not a factor in accepting a weld that is spot radiographed, so the Mandatory Appendix 4 charts are not laid over spot films. A reader who applies them will reject welds the code accepts. The report for a spot examination should cite UW-52 as its acceptance standard, and reserve Appendix 4 for joints the data report shows as fully radiographed.
What happens when a UW-52 spot radiograph fails?
Two additional spots are radiographed in the same weld increment, at locations away from the first. If both are acceptable, the increment is accepted once the defect found in the first spot has been repaired and the repair examined. If either additional spot fails, the whole increment is rejected and has to be dealt with as UW-52 directs. Sampling is kept separate for each welder or welding operator throughout.
Need this applied on your job?
Atlantis writes and reviews procedures to this code, inspects welds against it, and trains technicians in visual weld inspection.