How New API 650 Storage Tank Welds Are Examined, Tested and Accepted

API 650 decides what must be examined on a new welded tank and where, then borrows most of its accept or reject limits. Shell butt-weld radiographs are judged to ASME Section VIII Division 1 UW-51(b), magnetic particle and penetrant results to Section VIII Appendices 6 and 8, and visual limits, vacuum-box and other leak tests to API 650's own Section 8 rules.

API published a 14th Edition in August 2025. The paragraph references and values here come from the 13th Edition (March 2020) with Errata 1 (January 2021), which API's 2026 tank inspector examinations still use; the tank's data sheet or purchase order names the edition that governs, so check each value against it. Section 8 is the examination chapter, covering radiography, magnetic particle, ultrasonic, penetrant and visual examination and the vacuum and tracer-gas tests. Which welds get which method is decided mostly in the erection and testing rules of Section 7, and the informative Annex T collects those calls in one summary table. Ultrasonic examination may replace radiography with the Purchaser's approval, and is then judged under Annex U rather than UW-51(b). Once the tank is in service, repairs, alterations and reconstruction move under API 653, which sends many examination questions back to API 650.

Source: API Standard 650, Welded Tanks for Oil Storage, 13th Edition (March 2020) with Errata 1 (January 2021), as described here; the 14th Edition was published in August 2025: Section 7 (erection, including shell-to-bottom welds and testing of bottoms, reinforcing plates and shell), Section 8 (methods of examining joints: radiographic, magnetic particle, ultrasonic, liquid penetrant and visual examination, vacuum and tracer-gas testing), Annex T (NDE requirements summary) and Annex U (ultrasonic examination in lieu of radiography); ASME BPVC Section VIII Division 1 UW-51(b) and Mandatory Appendices 4, 6 and 8; ASME BPVC Section V Articles 2, 6, 7 and 10; API Standard 653 for tanks in service. Paragraph numbers differ between editions; confirm values against the edition and addenda the tank was ordered to.

Technically reviewed by Anoop Rayavarapu — ASNT NDT Level III (UT, RT, MT, PT, VT)
API 650 examination and acceptance by weld or test (new construction)
Weld or testWhat API 650 calls forAcceptance standard
Shell vertical butt welds, thinner plate 3/8 in. (10 mm) or lessSpot radiographs: one in the first 10 ft (3 m) of each type and thickness by each welder or operator, then one in each further 100 ft (30 m); 25 percent of spots at vertical-horizontal intersections; a random spot in each vertical joint of the bottom courseASME Section VIII Division 1 UW-51(b)
Shell vertical butt welds, over 3/8 in. to 1 in. (10 to 25 mm)As above, plus every vertical-horizontal intersection; two spots in each bottom-course vertical joint, one as close to the bottom as practicableUW-51(b)
Shell vertical butt welds, over 1 in. (25 mm)Full radiography of the joint, including all intersectionsUW-51(b)
Shell horizontal butt weldsOne spot in the first 10 ft (3 m) of each type and thickness, then further spots at the interval the standard setsUW-51(b)
Magnetic particle and penetrant examination wherever requiredTechnique to ASME Section V Article 7 (MT) or Article 6 (PT)Section VIII Division 1 Appendix 6 (paras. 6-3 to 6-5) or Appendix 8 (paras. 8-3 to 8-5)
Inside shell-to-bottom weld, first pass and final weldVisual, plus one of the methods the standard lists: MT, penetrant, vacuum box or penetrating oilAppendices 6 and 8 for MT and PT indications; no leak where a leak-type method is used
Bottom plate weldsVisual plus vacuum box, tracer gas or water testNo through-thickness leak
Reinforcing plate weldsPneumatic test through the telltale hole at up to 15 lbf/in.2 (100 kPa) gauge, with soap film or another leak-detecting solution on the weldsNo leak
Ultrasonic examination in place of radiographyPurchaser approval requiredAPI 650 Annex U, not UW-51(b)
Thickness is that of the thinner plate at the joint. Radiographic spot rules are summarised; the standard adds requirements for insert plates, openings near welds, annular plates and flush-type connections. Some annexes for small or special tanks change the radiography requirements; check the annex the tank is designed to. US customary units first, SI as the standard gives them.

What API 650 examines itself and what it hands to ASME

A tank standard written around large, field-erected shells could have invented its own film criteria, but API 650 chose not to. It takes the radiographic acceptance standard of ASME Section VIII Division 1, paragraph UW-51(b), and the magnetic particle and penetrant criteria of Division 1's Mandatory Appendices 6 and 8. What API 650 writes for itself is everything around those limits: which joints are examined, how many spot radiographs are taken and where they go, what happens when a spot fails, how bottoms, roofs and reinforcing plates are leak tested, and the visual limits for undercut, porosity and reinforcement.

That split matters when a contractor's procedure is reviewed. A procedure that cites Section V as its acceptance standard is wrong for the same reason it is wrong on a vessel: Section V covers technique only. A procedure that cites UW-52, the Division 1 spot radiography paragraph, is also wrong, because API 650 points to UW-51(b) even though its own shell radiography is a spot programme. The acceptance criteria by code hub explains how to place a tank among the other construction codes, and our Section VIII acceptance criteria guide covers UW-51(b) in its home context.

Radiography of shell butt welds: where the spots go

Shell radiography is driven by plate thickness, measured on the thinner plate at the joint. For vertical joints in plate up to 3/8 in. (10 mm), one spot radiograph is taken in the first 10 ft (3 m) of completed joint of each type and thickness welded by each welder or welding operator, then one in each additional 100 ft (30 m). At least a quarter of the selected spots must fall at junctions of vertical and horizontal joints, and each vertical joint in the bottom course gets a random spot as well. The standard also asks for an equal number of spots from the work of each welder or operator, so the sample says something about every hand on the job.

From 3/8 in. up to 1 in. (25 mm) the same pattern applies, and in addition every vertical-horizontal junction in that thickness range is radiographed, while bottom-course vertical joints get two spots, one placed as close to the bottom as practicable. Vertical joints in plate thicker than 1 in. are fully radiographed, junctions included. Horizontal joints start with one spot in the first 10 ft of each type and thickness, regardless of the number of welders, and continue at about one spot in each further 200 ft (60 m). Openings that interrupt shell seams, insert plates and annular-plate butt welds carry their own radiography rules, so a plan built only from the vertical-joint pattern will miss joints the standard requires.

Good practice is for the Purchaser's inspector to choose spot locations after welding rather than let them be marked in advance, and the film identification has to tie each radiograph to a joint, a location and a welder. Without that link, the limits of defective welding cannot be traced when a spot fails.

Judging the film, and what happens when a spot fails

Each radiograph is judged against UW-51(b). That paragraph rejects any indication characterised as a crack or as a zone of incomplete fusion or penetration, limits other elongated indications by length relative to thickness, limits groups of aligned indications by their total length within a stated length of weld, and sends rounded indications to the charts of Division 1 Mandatory Appendix 4. The numbers sit in Section VIII; read them from the Division 1 edition the tank standard references rather than from a summary sheet.

API 650 adds a limit on the weld surface at the radiograph location, because heavy reinforcement makes a film harder to interpret. Published summaries of Section 8 give the crown as flush or uniform and no more than 1/16 in. for plate up to 1/2 in., 3/32 in. over 1/2 to 1 in., and 1/8 in. over 1 in. The technique itself, including image quality indicators and density, is governed by ASME Section V Article 2.

When a spot shows unacceptable welding, or the radiograph does not show where the defective welding ends, two spots adjacent to it are radiographed. If those also fail, the standard continues outward until the limits of the defective welding are established, and the erector may instead replace all the welding done by that welder or operator on the joint. Repaired areas are radiographed again and judged to the same standard. A radiographic programme that stops at the first failed spot leaves the rest of that welder's seam unproven.

Visual acceptance: undercut, porosity and reinforcement

Every shell butt weld and every fillet weld is examined visually, and the visual limits are API 650's own. Undercut on vertical butt joints, vertical attachments, nozzle, manhole and flush-type opening attachment welds and the inside shell-to-bottom weld is limited to 1/64 in. (0.4 mm). Horizontal butt joints, horizontal attachments and annular-ring butt joints are allowed 1/32 in. (0.8 mm). The difference is long-standing: the 10th edition already set 1/64 in. for vertical and 1/32 in. for horizontal joints.

Surface porosity is limited to one cluster of one or more pores in any 4 in. (100 mm) of weld length, with no cluster wider than 3/32 in. (2.5 mm). Weld reinforcement on butt joints, on each side of the plate, depends on orientation and thickness: vertical joints are allowed 3/32 in. for plate up to 1/2 in., 1/8 in. over 1/2 to 1 in. and 3/16 in. over 1 in.; horizontal joints are allowed 1/8 in., 3/16 in. and 1/4 in. for the same ranges. Cracks, including crater cracks, and arc strikes in or next to the welds are rejected.

Visual work on tanks is easy to under-document. A report that records each joint, the measured undercut and reinforcement, and the orientation used to choose the limit lets a reviewer check the call. Examiners can build the skill through visual testing training.

Magnetic particle and penetrant examination

Surface methods appear throughout the standard rather than in one place. Annex T lists them against the welds that need them: the first pass of the inside shell-to-bottom weld (unless penetrant, vacuum box or penetrating oil is used instead), the completed shell-to-bottom weld as one of the options, flush-type connection welds after stress relief and before the hydrostatic test, permanent attachments and temporary weld removal areas on the higher-strength material groups, and completed welds of stress-relieved assemblies. Penetrant replaces magnetic particle where the material is not ferromagnetic, as on stainless steel tanks.

Technique follows ASME Section V Article 7 for magnetic particle and Article 6 for penetrant. Acceptance follows Section VIII Division 1 Mandatory Appendix 6, paragraphs 6-3 to 6-5, and Appendix 8, paragraphs 8-3 to 8-5: the relevance threshold, the linear and rounded definitions and the rejection rules for each. Our guide to ASME PT and MT acceptance criteria sets those out. In the United States our technicians perform magnetic particle weld inspection and penetrant testing of welds on tank work to these references.

Vacuum box, tracer gas and other tightness tests

Bottoms, roofs and reinforcing plates are proved by leak tests rather than by film. Bottom welds are tested along their full length by vacuum box, by tracer gas, or by a water test where the other two are not used. A vacuum box test follows a written procedure prepared by the tank manufacturer. The box applies a partial vacuum of 3 to 5 lbf/in.2 gauge (21 to 35 kPa, 6 to 10 in. Hg) over a solution-coated weld, and a second test at 8 to 10 lbf/in.2 (56 to 70 kPa, 16 to 20 in. Hg) can be used to find very small leaks. Each placement overlaps the previous one by at least 2 in. (50 mm), the metal surface must be between 40 F and 125 F (4 C and 52 C), the light at the examination point must be at least 100 fc (1000 lux), and the vacuum is held for at least 5 seconds or as long as viewing takes.

Acceptance is simple to state and easy to rush: bubbles that form and grow show air passing through the weld, and that is a rejectable leak. Tracer gas testing uses a gas and detector able to find leaks of 1 x 10-3 std cm3/s (1 x 10-4 Pa m3/s) or smaller, which suits large bottoms with long seams. Reinforcing-plate welds are tested by air at up to 15 lbf/in.2 (100 kPa) gauge through the telltale hole, with soap film on the welds, and the telltale holes are left open afterwards. The shell itself is proved by the hydrostatic test. Technique detail for bubble and tracer methods sits in ASME Section V Article 10.

Ultrasonic examination in place of radiography: Annex U

Ultrasonic examination may replace radiography of shell butt welds, annular plates and flush-type connection welds when the Purchaser approves it. The replacement is not a like-for-like swap of methods under the same criteria: Annex U sets its own requirements for the examination and its own acceptance standards, and UW-51(b) no longer applies to the welds examined that way. A contractor proposing ultrasonics in lieu of radiography should therefore submit a procedure written to Annex U, with the acceptance clause quoting the annex and edition.

Ultrasonic examination used for some other purpose, such as checking a suspect area found visually, is a different case: the standard leaves its acceptance criteria to agreement between the Purchaser and the Manufacturer, and that agreement should be written down before the examination. Atlantis does not carry out radiography in the United States. Where the tank standard and the Purchaser allow it, ultrasonic examination takes the volumetric role, and our ASNT Level III reviews the radiographs and RT procedures of the owner's licensed radiography contractor. The RT acceptance criteria by code guide compares the film standards side by side.

Mistakes in tank NDE packages, and what the records should show

Citing UW-52 because the programme is spot radiography. Counting spots per joint instead of per welder, type and thickness. Missing the intersection spots in the thicker plate range. Placing bottom-course spots away from the bottom where the standard asks for one close to it. Applying the 1/32 in. horizontal undercut limit to vertical joints. Running a vacuum box faster than the hold time, without overlap, or on a surface too cold for the solution. Accepting an ultrasonic replacement for radiography without the Purchaser's approval or without an Annex U procedure. Closing a failed spot without the adjacent spots.

A tank NDE record set that survives review states the edition, the plate thickness and joint type for each radiograph, the welder or operator, the spot location on a shell layout, and the result against UW-51(b); the vacuum level, overlap and temperature for each leak test; and the measured undercut and reinforcement for visual work. Procedures that carry these fields as mandatory entries, managed under document control such as procedures in Atlantis ERP, make the package easier to audit.

When the tank is in service: API 653 takes over

API 650 governs the tank until it is placed in service. From then on, inspection, repair, alteration and reconstruction come under API 653, still the 5th Edition (November 2014), which API's examination lists now show with Addenda 1 to 4 (the fourth issued in July 2025) and two errata; our API 653 overview summarises the standard. Repairs and alterations still draw on API 650 for many examination and acceptance requirements, so a repair procedure often cites both documents: API 653 for what has to be examined after the work, and API 650 or the ASME references it uses for whether the result is acceptable. The owner's API 653 authorized inspector decides on the results; inspection companies perform the examinations and report the data.

Thickness questions in service are judged differently again, by the minimum acceptable thickness the standard calculates for each course; see API 653 shell minimum thickness. For the inspection programme itself, our aboveground storage tank inspection page describes the external, ultrasonic and internal inspections and the data each one produces.

Where Atlantis fits

Atlantis's ASNT NDT Level III writes tank examination procedures with the spot plan, the acceptance references and the leak-test parameters taken from the edition on the tank's data sheet, and reviews contractor radiographs and leak-test records against them; see NDT procedure development. In the United States, Atlantis technicians are mobilised to the tank site for magnetic particle, penetrant, visual and ultrasonic work, including the shell thickness data an API 653 inspector relies on. On API 653 work the owner's authorized inspector makes the acceptance decisions, and Atlantis performs the NDE and reviews the data.

What radiographic acceptance standard does API 650 use?

ASME Section VIII Division 1, paragraph UW-51(b). Even though API 650 shell radiography is a spot programme, the standard does not use UW-52, the Division 1 spot radiography paragraph. UW-51(b) rejects cracks and zones of incomplete fusion or penetration, limits elongated indications and aligned groups, and judges rounded indications against Mandatory Appendix 4. API 650 adds its own limit on reinforcement at the radiograph location.

What undercut does API 650 allow?

1/64 in. (0.4 mm) on vertical butt joints, vertical attachments, nozzle, manhole and flush-type opening attachment welds and the inside shell-to-bottom weld, and 1/32 in. (0.8 mm) on horizontal butt joints, horizontal attachments and annular-ring butt joints. The tighter limit on vertical joints has been in the standard since at least the 10th edition. Measure undercut with a gauge and record the orientation used to choose the limit.

How is an API 650 vacuum box test performed and accepted?

To the manufacturer's written procedure, with a partial vacuum of 3 to 5 lbf/in.2 gauge over a weld coated with bubble solution, at least 2 in. overlap between placements, a metal temperature between 40 F and 125 F, at least 100 fc of light, and a hold of at least 5 seconds or the viewing time. Bubbles that form and grow show a through-thickness leak, which is rejected and repaired before retesting.

Can ultrasonic testing replace radiography on an API 650 tank?

Yes, with the Purchaser's approval, for the shell, annular plate and flush-type connection butt welds that would otherwise be radiographed. The examination and its acceptance then follow Annex U, not UW-51(b), so the procedure must be written to the annex. Where ultrasonics is used for another purpose, the acceptance criteria are agreed between the Purchaser and the Manufacturer before the work.

How many spot radiographs does an API 650 shell need?

It depends on plate thickness and on the number of welders. For vertical joints up to 3/8 in., one spot in the first 10 ft of each type and thickness per welder or operator, then one per further 100 ft, with a quarter of the spots at intersections and a random spot in each bottom-course vertical joint. Thicker plate adds every intersection and more bottom-course spots, and plate over 1 in. is fully radiographed.

Does API 650 or API 653 apply to a tank repair?

API 653 governs inspection, repair, alteration and reconstruction once a tank is in service, and it decides what must be examined after the work. Many of its acceptance questions are answered by API 650 or by the ASME references API 650 uses, so repair procedures often cite both. The owner's API 653 authorized inspector accepts the repair; the NDT contractor examines it and reports the results.

Request a consultation