{"slug":"/standards/rt-acceptance-criteria-by-code","title":"Radiographic Testing Acceptance Criteria: ASME, B31, AWS, API","description":"RT acceptance criteria compared: elongated, aligned and rounded indications under ASME VIII UW-51 and UW-52, B31.1, B31.3, API 1104, API 650 and AWS D1.1.","h1":"Radiographic Acceptance Criteria Compared: Elongated, Aligned and Rounded Indications by Code","answer":"Radiographic acceptance criteria come from the construction code, never from ASME Section V. On a fully radiographed Section VIII Division 1 joint, UW-51(b) rejects any crack or zone of incomplete fusion or penetration, and any other elongated indication longer than 1/4 in. for t up to 3/4 in., t/3 from 3/4 to 2-1/4 in., or 3/4 in. above 2-1/4 in.","expansion":"The same paragraph rejects aligned groups whose aggregate length exceeds t in a length of 12t, unless successive imperfections are more than 6L apart, and sends rounded indications to the charts in Mandatory Appendix 4. Spot radiography under UW-52 is judged more loosely and ignores rounded indications altogether. ASME B31.1 uses the same elongated-indication steps but judges porosity against Section I rather than Section VIII. B31.3 sets limits per imperfection and fluid service in Table 341.3.2. API 1104 works on individual and aggregate lengths in any 12 in. of pipeline weld, API 650 tank radiographs are judged to UW-51(b) even on a spot programme, and AWS D1.1 carries its own criteria for statically and cyclically loaded structures. Before any of those apply, the radiograph itself has to meet the technique and image-quality requirements; an unreadable film is not accepted or rejected, it is retaken.","source":"ASME BPVC Section VIII Division 1 (2023 edition): UW-51(b), UW-52(b) and (c), Mandatory Appendix 4; ASME BPVC Section I, Appendix A-250; ASME B31.1, para. 136.4; ASME B31.3-2022, Table 341.3.2; ASME BPVC Section V, Article 2 (technique and image quality); API Standard 1104 (22nd edition, with 49 CFR 192.7 and 195.3 incorporating the 21st), acceptance standards for radiography; API 650 (13th edition, the basis of the values here; the 14th edition was issued in August 2025), Section 8 and Annex T; AWS D1.1/D1.1M:2025, Clause 8. Confirm values against the edition your construction code, regulation or contract invokes.","table":{"caption":"Radiographic acceptance by indication type in four ASME documents","columns":["Indication","Section VIII Div 1, full RT (UW-51(b))","Section VIII Div 1, spot RT (UW-52(c))","B31.1 power piping (para. 136.4)","B31.3, severe cyclic conditions (Table 341.3.2)"],"rows":[["Crack","Rejected","Rejected","Rejected","Zero: no evident imperfection"],["Incomplete fusion or penetration","Rejected","Rejected","Rejected","Zero for lack of fusion and incomplete penetration"],["Slag or other elongated indication","Rejected over 1/4 in. (t to 3/4 in.), over t/3 (3/4 to 2-1/4 in.) or over 3/4 in. (above 2-1/4 in.)","Rejected over 2/3t; under 1/4 in. always acceptable, over 3/4 in. always rejected","Rejected beyond the same three thickness steps as UW-51(b)","Accepted up to Tw/3 long and up to 2.5 mm (3/32 in.) and Tw/3 wide"],["Aligned group","Rejected when the aggregate exceeds t in 12t, unless successive imperfections are more than 6L apart","Acceptable if the sum is no more than t in 6t and the longest are at least 3L apart","Rejected when the aggregate exceeds t in 12t (para. 136.4.5)","Accepted up to a cumulative Tw in any 12Tw of weld"],["Rounded indications (porosity)","Mandatory Appendix 4 charts","Not a factor","Section I Appendix A-250","Section VIII Div 1 Appendix 4"]],"note":"t is the weld thickness excluding allowable reinforcement (UW-51); Tw is the nominal wall thickness of the thinner component. In Normal and Category M fluid service B31.3 sets different, generally wider limits. API 1104, API 650 and AWS D1.1 are covered in the text."},"sections":[{"heading":"Image quality is the precondition, not a formality","paragraphs":["Every acceptance clause on this page assumes a radiograph that is fit to be read. For the ASME codes that means the technique and quality requirements of Section V Article 2: the image quality indicator selected for the material and thickness, placed where the article requires, with the required hole or wire visible; density within the article's limits across the area of interest; and the identification, location markers and film or digital image quality that let the image be tied to a weld and a position. If any of these fails, the right decision is a retake, not an evaluation of indications on a film that may be hiding them.","Reviewers see this step skipped more than any other. A report that lists indications and an accept decision without recording that the image quality indicator sensitivity and density were checked has not demonstrated that the weld was examined at the sensitivity the code assumes. See [Section V Article 2](/standards/asme-section-v-article-2) for the technique rules and the [image quality indicator glossary entry](/glossary/image-quality-indicator-iqi) for how hole-type and wire-type indicators differ."]},{"heading":"Digital radiographs: the limits stay, the proof of image quality changes","paragraphs":["Computed radiography with phosphor imaging plates and radiography with digital detector arrays have their own requirements within Section V Article 2, and moving a job from film to either one does not change the construction code's reject limits. What changes is how the image is shown to be fit for evaluation. The image quality indicator still has to be visible at the required sensitivity, but film density gives way to the digital image measures and display conditions that the article and the written procedure set, and the monitor, the viewing software and any processing applied to the image become part of the examination record.","Section VIII Division 1 is explicit about the film case: acceptable density together with visibility of the prescribed hole or wire of the image quality indicator is satisfactory evidence of compliance, and the geometric unsharpness provisions of Article 2, T-274.2, are to be used only as a guide for film-based radiography. That wording is a reminder that film rules do not carry across to digital images automatically. A procedure that converts a job to digital should state how image quality will be demonstrated and recorded before the first exposure, not after the first dispute. For castings, the ASTM film reference radiographs carry their own restriction on digital use."]},{"heading":"Full radiography under Section VIII Division 1","paragraphs":["UW-51(b) lists four reasons to reject a fully radiographed joint. The first is any indication characterised as a crack or zone of incomplete fusion or penetration, whatever its size. The second is any other elongated indication longer than 1/4 in. (6 mm) where t is up to 3/4 in. (19 mm), longer than t/3 where t runs from 3/4 in. to 2-1/4 in. (57 mm), or longer than 3/4 in. (19 mm) where t exceeds 2-1/4 in. Here t is the thickness of the weld excluding any allowable reinforcement. The third is a group of aligned indications whose aggregate length exceeds t within a length of 12t, unless the distance between successive imperfections exceeds 6L, where L is the length of the longest imperfection in the group. The fourth is rounded indications beyond the limits of Mandatory Appendix 4.","A worked case shows how the rules interact. On a 1 in. weld the longest acceptable single slag indication is about 0.33 in. Three slag lines of 0.3 in. each, sitting in a row within 12 in. of weld, total 0.9 in. and pass the group rule; add a fourth and the aggregate reaches 1.2 in., which fails unless the gaps between them exceed six times the longest indication. Each indication passes individually and the weld still fails. That is the point of the group rule, and it is the one interpreters most often forget to apply.","Appendix 4 handles porosity with charts rather than a single number. Its charts show the maximum acceptable concentration of rounded indications for each thickness range, and they represent full-scale 6 in. (150 mm) radiographs that are not to be enlarged or reduced. The appendix also sets the size below which a rounded indication is not counted and the largest size permitted, both scaled with thickness, so the interpreter reads the chart for the joint's thickness band rather than estimating."]},{"heading":"Spot radiography under UW-52: a sample judged by a different standard","paragraphs":["Spot radiography exists to check the welder's work, not to certify every inch of weld, and UW-52(c) judges it accordingly. Cracks and zones of incomplete fusion or penetration remain unacceptable. Slag inclusions and cavities are unacceptable when an indication is longer than 2/3t, with two fixed bounds for all thicknesses: indications shorter than 1/4 in. (6 mm) are acceptable and indications longer than 3/4 in. (19 mm) are not. Indications in line are acceptable when the sum of their longest dimensions does not exceed t within a length of 6t and the longest of them are separated by at least 3L of acceptable weld metal, where L is the length of the longest. Rounded indications are not a factor in the acceptability of welds that are not required to be fully radiographed.","Applying UW-51 limits to a spot film is a common and costly misreading in both directions. It rejects acceptable welds by counting porosity the code does not count, and it can accept welds that the spot rules would also accept but for the wrong reason, leaving no defensible record. The spot rules also carry consequences beyond the film: a failed spot is followed by two additional spots in the same weld increment, placed away from the first and chosen the same way, and failure there leads to radiography of the whole increment or its removal and rewelding. The [Section VIII Division 1 acceptance criteria guide](/standards/asme-section-viii-acceptance-criteria) covers the sampling and progressive steps in detail."]},{"heading":"B31.1 and Section I: the same length steps, different porosity charts","paragraphs":["Power piping under ASME B31.1 rejects cracks and zones of incomplete fusion or penetration, and uses the same three elongated-indication steps as UW-51(b): 1/4 in. up to 3/4 in. thick, t/3 to 2-1/4 in., and 3/4 in. beyond. It departs from the vessel code on porosity. B31.1 judges rounded indications against Appendix A-250 of Section I, the power boiler code, rather than against Section VIII Appendix 4. The two appendices are built on similar principles, but a B31.1 report that cites Appendix 4 has cited the wrong document, and an Authorized Inspector on boiler external piping will notice.","Section I's own Appendix A-250 limits the largest permissible rounded indication to 1/4t or 5/32 in. (4 mm), whichever is smaller, and treats aligned rounded indications as acceptable when the sum of their diameters is less than t in a length of 12t. The boiler code keeps its full radiographic acceptance rules in Part PW, which the [Section I acceptance criteria guide](/standards/asme-section-i-acceptance-criteria) explains, and power piping is covered in the [B31.1 acceptance criteria guide](/standards/asme-b31-1-acceptance-criteria)."]},{"heading":"B31.3: limits set per imperfection and per fluid service","paragraphs":["Process piping does not use a single rejection list. Table 341.3.2 gives each imperfection its own criterion and varies it with fluid service, so the same radiograph can be acceptable in Normal Fluid Service and rejectable under severe cyclic conditions. Under severe cyclic conditions cracks, lack of fusion and incomplete penetration are not permitted at all; slag, tungsten and other elongated indications are limited to an individual length of Tw/3, an individual width of 2.5 mm (3/32 in.) and Tw/3, and a cumulative length of Tw in any 12Tw of weld; and porosity is judged against Section VIII Division 1 Appendix 4.","Normal and Category M fluid service relax several of those limits, including porosity, where welds thicker than 6 mm (1/4 in.) may carry one and a half times the Appendix 4 concentration. Because the limits differ by column, a B31.3 radiographic procedure has to state which fluid service applies to each line, and the interpreter has to read the right column. The [B31.3 acceptance criteria guide](/standards/asme-b31-3-acceptance-criteria) sets out the full table and the random and progressive examination rules that decide how many welds are radiographed."]},{"heading":"API 1104, API 650 and AWS D1.1","paragraphs":["Pipeline girth welds are judged by length, not depth. API 1104 gives each discontinuity type its own designation and limits it by individual length, by aggregate length in any continuous 12 in. (300 mm) of weld and, for several types, by a share of total weld length. Porosity has separate rules for individual pore size relative to wall thickness and for distribution, and cracks are defects except small crater or star cracks within a stated length. Densities are read on the negative image, which matters for burn-through and internal concavity. The [API 1104 acceptance criteria guide](/blog/api-1104-weld-acceptance-criteria-pipeline) gives the limits; the regulation still incorporates an earlier edition than the one in print.","New storage tanks are built to API 650, whose Section 8 decides which shell butt welds are radiographed and where, and judges the radiographs against Section VIII Division 1 UW-51(b). The tank standard owns the sampling pattern; the vessel code owns the reject limits. One consequence surprises interpreters used to vessels: although tank shell radiography is a spot programme, API 650 points to the full-radiography paragraph, so rounded indications are evaluated against Appendix 4 on tank films, and a procedure citing UW-52 for a tank is wrong. See the [API 650 weld acceptance criteria guide](/standards/api-650-weld-acceptance-criteria).","Structural welds under AWS D1.1 are radiographed only where the contract documents call for it, and Clause 8 then applies its own criteria, which relate permitted discontinuity size and spacing to weld size and which differ between statically and cyclically loaded connections. A D1.1 film is not read against UW-51, and a vessel film is not read against D1.1."]},{"heading":"Repairs and re-radiography","paragraphs":["A rejected indication leads to repair, and the repair is judged again under the same paragraph. Section VIII Division 1 sends weld repairs to UW-38 and requires the repaired area to be re-examined; at the manufacturer's option the repaired weld may instead be examined ultrasonically under Mandatory Appendix 12, with the user's concurrence where the material is over 1 in. (25 mm) thick, which matters when a radiography crew is no longer available on site. On a spot-radiographed joint, repairing the failed spot does not close the question, because the additional spots in the same weld increment still have to be taken.","API 1104 handles repairs in a section of its own: repaired areas are re-examined by the means used before and must meet the same acceptance standards, cracks can be repaired only within limits, and a second repair of the same area needs its own qualified procedure. Under B31.3, a weld rejected in a random sample is repaired and re-examined, and the progressive rule adds further samples of the same welder's or operator's work, so a single failed radiograph can widen the programme considerably. Each repair film should carry an identification that ties it to the original film and the repair, so the reviewer can see both."]},{"heading":"Errors seen when radiographs are read against the wrong rules","paragraphs":["Measuring t with the reinforcement included, which inflates every length limit on a Section VIII joint. Evaluating rounded indications on a spot radiograph. Shrinking or enlarging an Appendix 4 chart to compare it with a film of a different length. Applying each elongated limit to single indications and never checking the group rule. Citing Section VIII Appendix 4 for porosity on B31.1 piping, or the Normal Fluid Service column of B31.3 on a line designated severe cyclic. Calling a straight, sharp-edged root indication slag when its position and profile point to incomplete penetration, which converts an absolute reject into a length check.","Process faults cause as many disputes as interpretation faults. Films are evaluated without recording image quality indicator sensitivity, density or the technique used; digital images are read on monitors that have not been checked as the procedure requires; and the interpreter's certification level and the code edition are missing from the report. A report that records the governing code, edition and paragraph, the image quality achieved, each indication with type, location and size, and the decision against a named limit can be audited. One that records only accept cannot."]},{"heading":"Keeping radiographs and examination records","paragraphs":["Division 1 makes the manufacturer retain a complete set of radiographic images and examination records, as described in Section V Article 2, for each vessel or vessel part: the images until the Inspector has signed the Manufacturer's Data Report, and the examination records as the Division requires. Owners often ask for longer retention by contract, particularly for equipment that will then be inspected under API 510 for decades, because a baseline radiograph is the only way to tell whether an indication found later was present at fabrication.","Digital images make long retention easier but bring controls of their own. The original image files should be kept unaltered, the viewing conditions documented, and any later reprocessing recorded as a separate evaluation instead of overwriting the first. A radiograph that cannot be traced to its weld, its technique and its interpreter is of little use at the next outage, however clear it looks on the screen."]},{"heading":"Radiographic testing compared with ultrasonic substitution","paragraphs":["Several of these codes let ultrasonic examination replace radiography on thicker welds, and the acceptance rules then change as well as the method. Section VIII Division 1 does it through UW-51(a)(4), B31.3 through its own ultrasonic paragraph and appendix, and API 650 through Annex U. The ultrasonic route brings its own criteria, so a contractor cannot carry the radiographic limits across. Our [ultrasonic testing acceptance criteria by code](/standards/ut-acceptance-criteria-by-code) guide compares those rules, and [RT versus UT for weld inspection](/blog/rt-vs-ut-weld-inspection) discusses which flaw types each method detects best."]},{"heading":"Where Atlantis fits","paragraphs":["To be plain about scope: Atlantis does not perform radiography in the United States; where the code allows, ultrasonic testing is used for volumetric examination, and our ASNT Level III can review radiographs and RT procedures produced by a licensed contractor. That review checks the technique and image quality first, then each indication against the code, edition and paragraph the contract names. See [NDT Level III consulting](/consulting/ndt-consulting-level-iii) and [NDT procedure development](/consulting/ndt-technical-procedure-development).","Inspectors who interpret radiographs, or who supervise those who do, can build the theory through [radiographic testing training](/radiographic-testing-training) built on SNT-TC-1A, and owners can return the acceptance reference to every weld record with [NDT reports in Atlantis ERP](/erp/apps/ndt-reports). For the full map of which code governs which asset, start at the [NDT acceptance criteria hub](/standards/ndt-acceptance-criteria-by-code)."]}],"facets":[{"q":"What are the RT acceptance criteria in ASME Section VIII Division 1?","a":"For fully radiographed joints, UW-51(b) rejects cracks and zones of incomplete fusion or penetration; other elongated indications longer than 1/4 in. (t to 3/4 in.), t/3 (t from 3/4 to 2-1/4 in.) or 3/4 in. (t beyond 2-1/4 in.); aligned groups exceeding t in 12t unless more than 6L apart; and rounded indications beyond Mandatory Appendix 4. Spot radiography follows UW-52(c) instead."},{"q":"How does spot radiography acceptance differ from full radiography?","a":"UW-52(c) allows slag inclusions and cavities up to 2/3t, with indications under 1/4 in. always acceptable and over 3/4 in. always rejected, and judges aligned indications over a length of 6t with 3L separation. Rounded indications are not evaluated at all. Cracks and incomplete fusion or penetration are rejected under both paragraphs."},{"q":"What does t in a length of 12t mean on a radiograph?","a":"It is the aligned-indication rule in UW-51(b) and B31.1. Measure the weld thickness t, look along a weld length of twelve times t, and add the lengths of indications lying in a line. If the total exceeds t the group is rejected, unless the gap between successive indications is more than six times the longest one."},{"q":"Which porosity charts does ASME B31.1 use?","a":"Appendix A-250 of ASME Section I, the power boiler code, not Section VIII Appendix 4. Section I limits the largest permissible rounded indication to 1/4t or 5/32 in., whichever is smaller, and accepts aligned rounded indications only when their diameters total less than t in a length of 12t. A B31.1 report should cite A-250 by name."},{"q":"Can a radiograph be evaluated if the image quality requirements are not met?","a":"No. Under the ASME codes the radiograph must first satisfy Section V Article 2: the specified image quality indicator sensitivity, density limits and identification. A film that misses them cannot show that the weld was examined at the sensitivity the acceptance limits assume, so it is retaken rather than accepted or rejected."},{"q":"Does API 650 have its own radiographic acceptance limits?","a":"No. API 650 decides which tank shell welds are radiographed, how many spots are taken and where, and judges the radiographs against ASME Section VIII Division 1 UW-51(b), including its Appendix 4 rounded-indication rule, even though the tank programme is spot radiography. Where ultrasonic examination replaces radiography with the Purchaser's approval, Annex U applies instead."}],"faq":[{"q":"What are the RT acceptance criteria in ASME Section VIII Division 1?","a":"For fully radiographed joints, UW-51(b) rejects cracks and zones of incomplete fusion or penetration; other elongated indications longer than 1/4 in. (t to 3/4 in.), t/3 (t from 3/4 to 2-1/4 in.) or 3/4 in. (t beyond 2-1/4 in.); aligned groups exceeding t in 12t unless more than 6L apart; and rounded indications beyond Mandatory Appendix 4. Spot radiography follows UW-52(c) instead."},{"q":"How does spot radiography acceptance differ from full radiography?","a":"UW-52(c) allows slag inclusions and cavities up to 2/3t, with indications under 1/4 in. always acceptable and over 3/4 in. always rejected, and judges aligned indications over a length of 6t with 3L separation. Rounded indications are not evaluated at all. Cracks and incomplete fusion or penetration are rejected under both paragraphs."},{"q":"What does t in a length of 12t mean on a radiograph?","a":"It is the aligned-indication rule in UW-51(b) and B31.1. Measure the weld thickness t, look along a weld length of twelve times t, and add the lengths of indications lying in a line. If the total exceeds t the group is rejected, unless the gap between successive indications is more than six times the longest one."},{"q":"Which porosity charts does ASME B31.1 use?","a":"Appendix A-250 of ASME Section I, the power boiler code, not Section VIII Appendix 4. Section I limits the largest permissible rounded indication to 1/4t or 5/32 in., whichever is smaller, and accepts aligned rounded indications only when their diameters total less than t in a length of 12t. A B31.1 report should cite A-250 by name."},{"q":"Can a radiograph be evaluated if the image quality requirements are not met?","a":"No. Under the ASME codes the radiograph must first satisfy Section V Article 2: the specified image quality indicator sensitivity, density limits and identification. A film that misses them cannot show that the weld was examined at the sensitivity the acceptance limits assume, so it is retaken rather than accepted or rejected."},{"q":"Does API 650 have its own radiographic acceptance limits?","a":"No. API 650 decides which tank shell welds are radiographed, how many spots are taken and where, and judges the radiographs against ASME Section VIII Division 1 UW-51(b), including its Appendix 4 rounded-indication rule, even though the tank programme is spot radiography. Where ultrasonic examination replaces radiography with the Purchaser's approval, Annex U applies instead."}]}