{"slug":"/standards/aws-d1-5-bridge-weld-acceptance-criteria","title":"AWS D1.5 Bridge Weld Acceptance Criteria (2025 Edition)","description":"How AASHTO/AWS D1.5 accepts bridge welds: 2025 undercut tolerances, tension vs compression testing, UT indication classes, fracture-critical rules, D1.1 contrasts.","h1":"Inspecting and Accepting Steel Bridge Welds Under AASHTO/AWS D1.5","answer":"AASHTO/AWS D1.5, the Bridge Welding Code, sets weld acceptance in its inspection clause and adds fracture-critical rules in Clause 12. Cracks are never accepted. Welds in tension or stress reversal face stricter testing and acceptance than welds in compression, and the 2025 edition replaced the old undercut limits with three tolerances, 0.01 in., 1/8 in. and 1/16 in., applied toe by toe.","expansion":"The current code is AASHTO/AWS D1.5M/D1.5:2025, the 9th edition, which superseded the 2020 edition and folded in the 2023 and 2024 AASHTO interim revisions. It covers welded highway bridges of carbon and low-alloy constructional steel designed to AASHTO or AREMA requirements. Clauses 1 to 9 carry the general rules, Clauses 10 and 11 are deliberately empty because the D1.1 subjects they mirror do not apply to bridges, and Clause 12 governs fracture-critical members. Owner agencies adopt editions on their own timetable, so the contract documents and the state specifications decide which edition and supplements apply to a girder. D1.5 acceptance is a workmanship judgement rather than a fitness-for-purpose one: NCHRP Research Report 908 observed that the code's criteria are not based on how a discontinuity affects fatigue or fracture performance, and proposed changes built on phased-array ultrasonics.","source":"AASHTO/AWS D1.5M/D1.5:2025 Bridge Welding Code, 9th edition (supersedes D1.5M/D1.5:2020 and the 2023 and 2024 interim revisions): inspection clause, including the visual criteria in 8.26.1.5 (undercut), repair of nonconforming undercut in 5.7.2.5, and Clause 12 (fracture-critical members); earlier text referred to where noted: D1.5:2020 8.26.1.5 and 5.7.2.2, D1.5:2020 Clause 12 (Fracture Control Plan for Nonredundant Members), D1.5:2002 6.7.1, 6.7.2 and Table 6.3; NCHRP Research Report 908 (2019). AWS D1.1/D1.1M for comparison. The edition and supplements in the owner agency's contract govern; confirm values against that edition.","table":{"caption":"Key D1.5 acceptance rules, with the edition each comes from","columns":["Item","D1.5 rule","Edition note"],"rows":[["Undercut at a toe transverse to primary tensile stress","0.01 in. maximum, including groove welds in tension flanges and tension zones of webs; on a transverse fillet weld, only the toe on the tension component","Same value in 2020 and 2025 (8.26.1.5)"],["Undercut at corners of stiffeners and connection plates","1/8 in. maximum","New tolerance in 2025"],["Undercut everywhere else","1/16 in. maximum, including the toes of transverse fillet welds that sit on stiffeners and connection plates","2025; generally replaces the 2020 value of 1/32 in."],["Nonconforming undercut, toe transverse to tension","Ground smooth if the result stays within a depth limit set by plate thickness (1/32 in. for plate up to 1 in., rising to 1/8 in. over 2 in.); otherwise repaired by welding; grinding may not leave less than 98 percent of the nominal net section","2025 (5.7.2.5); 2020 allowed repair by welding only (5.7.2.2)"],["Nonconforming undercut, toe parallel to tension or in compression","Ground smooth if no deeper than 1/8 in. after grinding, whatever the thickness; otherwise repaired by welding","2025 (5.7.2.5)"],["Cracks","Rejected, whatever the size or method that finds them","All editions"],["Radiography of fracture-critical member welds","Hole-type image quality indicators; wire-type IQIs not permitted","2020 (Clause 12 and the inspection clause)"],["Lead inspector on fracture-critical work","At least three years in steel bridge construction or fabrication, and a current or former AWS CWI or an engineer or technician acceptable to the engineer of record; makes the final acceptance determination for FCM welds","2020 (Clause 12)"]],"note":"Undercut is assessed toe by toe, for each base metal component the weld touches. Values in US customary units as the code states them; the code also carries SI units. Read the numbers from the edition the contract invokes."},"sections":[{"heading":"Edition, scope and clause layout","paragraphs":["D1.5 is a joint AASHTO and AWS code, and its editions arrive on a different rhythm from D1.1. The 9th edition, D1.5M/D1.5:2025, replaced the 8th edition of 2020 and absorbed the interim revisions AASHTO had issued in 2023 and 2024. Its clause layout mirrors D1.1: the general body of rules runs from Clause 1 to Clause 9, the inspection rules sit in Clause 8, Clauses 10 and 11 are left without provisions because their D1.1 counterparts have no bridge application, and Clause 12 holds the requirements for fracture-critical members. A procedure or inspection plan written to the 2015 edition will cite clause numbers that no longer exist.","Scope is narrower than the name suggests: welded highway bridges built from carbon and low-alloy constructional steels, designed to AASHTO or AREMA requirements. State departments of transportation adopt editions on their own timetable and add supplements, so the contract documents settle which edition governs a fabrication shop's work. The [AWS D1.5 summary](/standards/aws-d1-5) covers the code in general; this guide covers how welds are inspected and accepted, and the [acceptance criteria by code hub](/standards/ndt-acceptance-criteria-by-code) shows where bridges sit beside buildings, vessels, piping and tanks."]},{"heading":"Which welds get which test: tension, compression and fillet welds","paragraphs":["Bridge members carry repeated live load, so D1.5 sorts welds by the stress the design says they carry. For decades the code's testing rules followed one pattern, set out in the 2002 text as Section 6.7: radiography for complete joint penetration groove welds subject to calculated tension or stress reversal, ultrasonic testing for complete joint penetration welds in corner joints, a choice of radiography or ultrasonics for complete joint penetration welds subject to compression or shear, and magnetic particle testing of fillet and partial joint penetration welds. The tension or compression designation therefore has to come from the contract drawings before the inspection plan can be written.","The 2020 revision gathered the methods and testing frequencies into a table in the inspection clause and placed the duty to perform NDT on welds to primary components of main members on the contractor. Where partial testing applies, the inspector picks the locations after welding is finished, which stops a fabricator from steering the sample toward its best work. Read the table in the edition your contract names for extent, permitted method substitutions and the frequency for each weld type, rather than carrying percentages over from an older procedure.","Phased array is not automatically a substitute for the conventional ultrasonic technique the code describes. NCHRP Research Report 908 set out guidelines and proposed code changes for evaluating complete joint penetration bridge welds with enhanced ultrasonic methods, and owner agencies differ on what they accept. Confirm in writing whether the edition and the owner permit the technique and which acceptance rules then apply."]},{"heading":"Visual acceptance and the 2025 undercut tolerances","paragraphs":["Visual inspection is the first acceptance step on every weld, and the 2025 edition changed its best-known number. The 2020 edition's subclause 8.26.1.5 set two undercut tolerances: 0.01 in. where the undercut was transverse to tensile stress, and 1/32 in. in all other cases, which matched the D1.1 limits for cyclically loaded connections. The 2025 subclause has three. The 0.01 in. limit still applies to welds transverse to primary tensile stress, including groove welds in tension flanges and in the tension zones of webs, and to fillet welds transverse to tension, but on a fillet weld only at the toe that sits directly on the tension component.","A new 1/8 in. tolerance applies at the corners of stiffeners and connection plates. Everywhere else the limit is 1/16 in., which generally replaces the old 1/32 in. value; that includes the toe of a transverse fillet weld that lands on a stiffener or connection plate rather than on the tension flange. The code's commentary illustrates the toe-by-toe split, and the change means undercut is now assessed separately for each base metal component the weld touches, not once per weld.","Inspectors who learned the 2020 numbers need to reset. Take a fillet weld joining a transverse stiffener to a tension flange: the 2020 wording did not separate its two toes, so it could be read as putting the whole weld under the 0.01 in. limit, which would reject 1/32 in. of undercut on the stiffener side. Under 2025 the flange-side toe stays at 0.01 in., while the stiffener-side toe is judged at 1/16 in. and the same reading passes. Recording which toe was measured is now part of a defensible visual record. The [visual testing training](/visual-testing-training) course covers gauge use and record keeping for this kind of call."]},{"heading":"Repairing nonconforming undercut under the 2025 rules","paragraphs":["The 2020 edition sent nonconforming undercut to repair by welding under subclause 5.7.2.2, although its commentary already observed that light grinding is generally better than a cosmetic weld repair. The 2025 edition makes grinding the first treatment under subclause 5.7.2.5. Undercut within the allowable depths is ground to a smooth surface, and grinding may not reduce the net cross section below 98 percent of the nominal area, a limit the code uses elsewhere too.","For weld toes transverse to tension, the depth allowed after grinding depends on plate thickness, from 1/32 in. for plate up to 1 in. thick to 1/8 in. for plate over 2 in. thick. On a 1 in. plate, undercut deeper than 0.01 in. is ground, and the result must be smooth and no deeper than 1/32 in., or the toe is repaired by welding; undercut already deeper than 1/32 in. goes straight to a weld repair. For toes parallel to tension or in compression, the ground undercut may not be deeper than 1/8 in., whatever the thickness. Anything beyond those depths is repaired by welding under 5.7.2.5(2), and the repaired area is inspected again against the visual criteria."]},{"heading":"Ultrasonic acceptance: indication rating, classes and weld quarters","paragraphs":["D1.5 shares D1.1's way of judging ultrasonic indications. The technician brings the maximum echo from a discontinuity to a reference line, and the gain readings are combined into an indication rating in decibels that accounts for the calibration reference and the sound path attenuation. That rating, the probe angle and the weld thickness place the indication in one of four classes. Class A is rejected at any length and Class D is accepted at any length; Classes B and C are accepted or rejected on length. Our guide to [AWS D1.1 UT acceptance criteria](/blog/aws-d1-1-ut-acceptance-criteria-explained) walks through the rating arithmetic, which is the part most often done wrong.","Where D1.5 departs is in how much a tension weld is allowed. The code has separate acceptance tables for welds in tension and in compression, and in the tension table, as published in the 2002 edition, a Class C indication in the top or bottom quarter of the weld thickness is held to a shorter length than the same indication in the middle half. Near-surface flaws matter more in fatigue, which is why the quarter in which an indication lies has to be recorded, not just its depth. Read the dB boundaries and length limits from the edition in force; they differ by thickness band and probe angle.","The ultrasonic procedure in D1.5 is the code's own, not ASME Section V, and it fixes the calibration blocks, probe angles, scanning patterns and the transducer movement used to maximise each echo. A technician who has worked mostly to vessel codes needs specific practice before rating bridge welds; see [ultrasonic testing training](/ultrasonic-testing-training) and our comparison of [UT acceptance criteria by code](/standards/ut-acceptance-criteria-by-code)."]},{"heading":"Radiographic acceptance and image quality","paragraphs":["On a radiograph, D1.5 rejects any crack. Other discontinuities, such as porosity and fusion-type indications, are judged by a combination of their length, the size of the weld and their spacing, with tension welds held to tighter limits than compression welds. The limits are presented graphically, so an interpreter measures each indication and its spacing and reads acceptability from the chart for the stress category and weld size.","Image quality rules are part of acceptance in practice: a film that does not show the required image quality indicator sensitivity cannot be accepted. On fracture-critical member welds, the 2020 edition requires hole-type image quality indicators and does not permit wire-type indicators. Atlantis does not perform radiography in the United States. Where the bridge code and the owner agency allow ultrasonic testing for the volumetric examination, that is the method Atlantis uses, and its ASNT Level III can review radiographs and RT procedures prepared by the fabricator's licensed radiography contractor. The guide to [RT acceptance criteria by code](/standards/rt-acceptance-criteria-by-code) compares the bridge chart approach with the vessel and piping codes."]},{"heading":"Fracture-critical members and the Fracture Control Plan","paragraphs":["Clause 12 applies to fracture-critical members, which the 2020 edition defines, following the AASHTO LRFD specifications, as steel primary members or portions of them subject to tension whose failure would probably cause part or all of the bridge to collapse. The Fracture Control Plan does not change the visual or NDT acceptance tables so much as tighten everything that leads up to a weld: base metal, consumables, procedures, processes and the people who inspect.","In the 2020 edition, base metal ordered for these members comes with Charpy test results at the temperature the engineer specifies, and all base metal surfaces and edges are inspected when the steel arrives. Consumables must be heat or lot tested by the manufacturer and come from quality programmes audited by ABS, Lloyd's Register or ASME, and fillers and fluxes other than SMAW electrodes carry a diffusible hydrogen designator of H4, H8 or H16 for base metal with a specified yield of 50 ksi or less. Prequalified procedures are allowed only for SMAW with E7016, E7018, E7018-1 and E8018-X electrodes; SAW, FCAW and GMAW groove procedures need qualification tests, including Charpy tests, generated within a year of the start of fracture-critical production welding. Electroslag and electrogas welding are not permitted on these members.","Inspection is tightened too. The plan names lead inspectors with at least three years of steel bridge construction or fabrication experience who are current or former AWS Certified Welding Inspectors, or engineers or technicians acceptable to the engineer of record, and the lead inspector makes the final determination on whether fracture-critical member welds are acceptable. The engineer reviews and approves the plan itself. Inspectors working toward that role can prepare through [AWS CWI exam preparation](/aws-cwi-training); the certification itself is awarded by AWS."]},{"heading":"How D1.5 differs from D1.1","paragraphs":["D1.1 sorts connections into statically and cyclically loaded and applies a different column of limits to each. D1.5 assumes repeated loading throughout and instead sorts welds by tension or stress reversal versus compression, then adds the fracture-critical layer on top. In their 2020 editions the two codes' undercut numbers matched for cyclically loaded tension welds, which let shops working to both use one checklist. D1.1 now has its own 2025 edition with its own undercut table, and D1.5's toe-by-toe tolerances and grinding treatments belong to the bridge code alone, so a structural steel checklist built on the [AWS D1.1 acceptance criteria](/blog/aws-d1-1-weld-acceptance-criteria-comprehensive-guide) should not be reused on a bridge girder without checking every limit.","Other differences run through qualification and scope. D1.1 permits a wide range of prequalified procedures; D1.5's fracture-critical rules restrict prequalification to shielded metal arc welding, and the code is written around bridge steels rather than the full structural range. D1.1's clauses on tubular structures and on strengthening and repairing existing structures have no D1.5 counterpart, which is why those clause numbers are empty in the bridge code. The [AWS D1.1 summary](/standards/aws-d1-1) covers the building code itself."]},{"heading":"Records and recurring mistakes on bridge work","paragraphs":["A D1.5 inspection record that will satisfy an owner agency identifies the member, the weld and its location on the shop drawing, whether the weld is in tension, stress reversal or compression, whether the member is fracture critical, the code edition and any state supplement, and the method and procedure. Visual entries give measured undercut for each toe and the tolerance applied; ultrasonic entries give the indication level, reference level, attenuation factor, rating, class, length and the quarter of the thickness in which the indication lies; repairs are traced to re-inspection.","Mistakes that recur: applying the 2020 undercut values to work contracted under the 2025 edition; measuring undercut once per weld instead of per toe; rating an ultrasonic indication with the compression table on a tension flange splice; leaving the quarter location off the report; using wire-type image quality indicators on fracture-critical welds; accepting a fabricator-chosen sample where the inspector should pick locations after welding; and copying a D1.1 checklist onto bridge work. Each is cheaper to prevent in the procedure than to argue about after the girder is painted; see [procedure qualification and demonstration](/consulting/ndt-procedure-qualification-demonstration) and our general notes on [bridge and structural steel NDT](/blog/bridge-and-structural-steel-inspection)."]},{"heading":"Where Atlantis fits","paragraphs":["Atlantis's ASNT NDT Level III prepares D1.5 ultrasonic, magnetic particle and visual procedures with acceptance clauses tied to the edition and stress category on the contract, demonstrates them on representative joints, and reviews fabricators' inspection records and radiographs. The written practice and qualification records an owner agency asks to see are covered by our [NDT Level III documentation](/consulting/ndt-level-iii-documentation) service. In the United States our technicians are mobilised to the shop or site for [ultrasonic weld inspection](/ultrasonic-weld-inspection), [magnetic particle weld inspection](/magnetic-particle-weld-inspection), penetrant and visual examination."]}],"facets":[{"q":"What undercut does AWS D1.5 allow in the 2025 edition?","a":"Three tolerances, assessed toe by toe. Up to 0.01 in. where the weld is transverse to primary tensile stress, including the tension-side toe of a transverse fillet weld; up to 1/8 in. at the corners of stiffeners and connection plates; and up to 1/16 in. everywhere else, which generally replaces the 2020 value of 1/32 in. Undercut beyond tolerance is ground smooth within set depths or repaired by welding."},{"q":"Which bridge welds does D1.5 require to be tested by RT or UT?","a":"The code bases testing on the design stress. Its long-standing pattern, in the 2002 text, was radiography of complete joint penetration welds in tension or stress reversal, ultrasonics for complete joint penetration corner joints, either method for welds in compression or shear, and magnetic particle testing of fillet and partial joint penetration welds. Since 2020 the methods and frequencies sit in a table in the inspection clause."},{"q":"How are ultrasonic indications accepted under D1.5?","a":"Each indication gets a decibel rating from the indication level, the reference level and an attenuation correction. The rating, probe angle and weld thickness place it in Class A, B, C or D: Class A is rejected and Class D accepted at any length, while B and C are judged on length. Tension welds have their own table, and Class C indications near the top or bottom surface face shorter length limits."},{"q":"What is a fracture-critical member under D1.5?","a":"In the 2020 edition, a steel primary member or portion of one subject to tension whose failure would probably cause part or all of the bridge to collapse, following the AASHTO LRFD definition. Clause 12, the Fracture Control Plan, applies to these members, tightening base metal toughness, consumable control, procedure qualification, permitted processes and inspector qualifications. The engineer reviews and approves the plan."},{"q":"Is AWS D1.5 stricter than AWS D1.1?","a":"For bridges, generally yes, but the codes are organised differently rather than one being a tighter copy of the other. D1.5 sorts welds by tension or compression and adds fracture-critical rules, and its 2025 undercut tolerances and grinding treatments are its own. D1.1 sorts connections into statically and cyclically loaded. Use the code the contract names; mixing their criteria is a common audit finding."},{"q":"Who decides whether a fracture-critical bridge weld is acceptable?","a":"Under the 2020 Fracture Control Plan, the lead inspector named in the plan makes the final determination on fracture-critical member welds. That person needs at least three years of steel bridge construction or fabrication experience and must be a current or former AWS CWI, or an engineer or technician acceptable to the engineer of record. NDT technicians report the indications against the code; the lead inspector decides."}],"faq":[{"q":"What undercut does AWS D1.5 allow in the 2025 edition?","a":"Three tolerances, assessed toe by toe. Up to 0.01 in. where the weld is transverse to primary tensile stress, including the tension-side toe of a transverse fillet weld; up to 1/8 in. at the corners of stiffeners and connection plates; and up to 1/16 in. everywhere else, which generally replaces the 2020 value of 1/32 in. Undercut beyond tolerance is ground smooth within set depths or repaired by welding."},{"q":"Which bridge welds does D1.5 require to be tested by RT or UT?","a":"The code bases testing on the design stress. Its long-standing pattern, in the 2002 text, was radiography of complete joint penetration welds in tension or stress reversal, ultrasonics for complete joint penetration corner joints, either method for welds in compression or shear, and magnetic particle testing of fillet and partial joint penetration welds. Since 2020 the methods and frequencies sit in a table in the inspection clause."},{"q":"How are ultrasonic indications accepted under D1.5?","a":"Each indication gets a decibel rating from the indication level, the reference level and an attenuation correction. The rating, probe angle and weld thickness place it in Class A, B, C or D: Class A is rejected and Class D accepted at any length, while B and C are judged on length. Tension welds have their own table, and Class C indications near the top or bottom surface face shorter length limits."},{"q":"What is a fracture-critical member under D1.5?","a":"In the 2020 edition, a steel primary member or portion of one subject to tension whose failure would probably cause part or all of the bridge to collapse, following the AASHTO LRFD definition. Clause 12, the Fracture Control Plan, applies to these members, tightening base metal toughness, consumable control, procedure qualification, permitted processes and inspector qualifications. The engineer reviews and approves the plan."},{"q":"Is AWS D1.5 stricter than AWS D1.1?","a":"For bridges, generally yes, but the codes are organised differently rather than one being a tighter copy of the other. D1.5 sorts welds by tension or compression and adds fracture-critical rules, and its 2025 undercut tolerances and grinding treatments are its own. D1.1 sorts connections into statically and cyclically loaded. Use the code the contract names; mixing their criteria is a common audit finding."},{"q":"Who decides whether a fracture-critical bridge weld is acceptable?","a":"Under the 2020 Fracture Control Plan, the lead inspector named in the plan makes the final determination on fracture-critical member welds. That person needs at least three years of steel bridge construction or fabrication experience and must be a current or former AWS CWI, or an engineer or technician acceptable to the engineer of record. NDT technicians report the indications against the code; the lead inspector decides."}]}